300
General purpose / Super impact strength |
| Properties |
Test Method |
Test Condition |
Units |
300 |
| Tensile Strength |
ASTM-D638 |
23 C/
50%RH |
MPa
kg/cm2
|
39
400 |
Tensile Elongation
at Break |
23 C/
50%RH |
% |
>50 |
| Flexural Strength |
ASTM-D790 |
23 C/
50%RH |
MPa
kg/cm2
|
57
580 |
| Flexural Modulus |
23 C/
50%RH |
MPa
kg/cm2
|
1,810
18,500 |
| Izod Impact
Strength |
ASTM-D256 |
23 C
12.7mm
V-notched |
J/m
kg cm/cm
|
333
34 |
0 C
12.7mm
V-notched |
206
21 |
-30 C
12.7mm
V-notched |
147
15 |
23 C
3.2mm
V-notched |
J/m
kg cm/cm
|
343
35 |
0 C
3.2mm
V-notched |
235
24 |
-30 C
3.2mm
V-notched |
157
16 |
Distortion Temperature
Under Load |
ASTM-D648 |
6.4mm
1.82MPa |
C |
84 |
| Rockwell Hardness |
ASTM-D785 |
23 C/
50%RH |
R-SCALE |
100 |
| Melt Flow Rate |
ISO-1133 |
220 C/98N |
g/10min |
10 |
| Specific Gravity |
ASTM-D792 |
23 C/
50%RH |
- |
1.04 |
Coefficient of Linear
Thermal Expansion |
ASTM-D696 |
- |
C-1 |
8.3 10-5 |
| Ball Pressure
Temperature |
C |
90 |
| Flammability |
UL94
File No.E41797 |
HB equivalent |
| Mold Shrinkage |
% |
0.4-0.6 |
|
| Note ; These values are typical data for
this product under specific test conditions and not intended
for use as limiting specifications. |
|
|
|
|